Composition
Table 1. Typical composition ranges for 304-grade stainless steel
| Grade | C | Mn | Si | P | S | Cr | Mo | Ni | N | |
|---|---|---|---|---|---|---|---|---|---|---|
| 304 | min. max. | - 0.08 | - 2.0 | - 0.75 | - 0.045 | - 0.030 | 18.0 20.0 | - | 8.0 10.5 | - 0.10 |
| 304L | min. max. | - 0.030 | - 2.0 | - 0.75 | - 0.045 | - 0.030 | 18.0 20.0 | - | 8.0 12.0 | - 0.10 |
| 304H | min. max. | 0.04 0.10 | - 2.0 | - 0.75 | -0.045 | - 0.030 | 18.0 20.0 | - | 8.0 10.5 | - |
Mechanical Properties
Table 2. Typical mechanical properties of 304-grade stainless steel
| Grade | Tensile Strength (MPa) min | Yield Strength 0.2% Proof (MPa) min | Elongation (% in 50 mm) min | Hardness | |
|---|---|---|---|---|---|
| Rockwell B (HR B) max | Brinell (HB) max | ||||
| 304 | 515 | 205 | 40 | 92 | 201 |
| 304L | 485 | 170 | 40 | 92 | 201 |
| 304H | 515 | 205 | 40 | 92 | 201 |
304H also requires a grain size of ASTM No 7 or coarser.
Physical Properties
Table 3. Typical physical properties of 304-grade stainless steel in the annealed condition
| Grade | Density (kg/m3) | Elastic Modulus (GPa) | Mean Coefficient of Thermal Expansion (μm/m/°C) | Thermal Conductivity (W/m.K) | Specific Heat 0-100 °C (J/kg.K) | Electrical Resistivity (nΩ.m) | |||
|---|---|---|---|---|---|---|---|---|---|
| 0-100 °C | 0-315 °C | 0-538 °C | at 100 °C | at 500 °C | |||||
| 304/L/H | 8000 | 193 | 17.2 | 17.8 | 18.4 | 16.2 | 21.5 | 500 | 720 |