SUS304H Stainless Steel: High-Temperature Grade Guide
Feb 27, 2026
Leave a message
What Is SUS304H Stainless Steel?
SUS304H is the Japanese Industrial Standard designation for the high-carbon variant of grade 304 austenitic stainless steel, with a controlled carbon range of 0.04 to 0.10 percent. The H suffix indicates that the grade is intended for high-temperature service: the elevated carbon content provides creep strength through solid-solution and carbide strengthening, which standard SUS304 with its 0.08 percent maximum carbon does not guarantee at elevated temperature.
The equivalent designations are UNS S30409 and TP304H under ASTM A240, A312 and A213. The grade is covered by JIS G4303 for stainless steel bars and JIS G4304 for hot-rolled stainless steel plate. EN 10088-2 does not list a direct 304H equivalent; European projects commonly cross-reference the X6CrNi18-11 chemistry for high-temperature tube applications, with the carbon range specified to ASTM TP304H.
Chemical Composition of SUS304H
The table below compares the heat-analysis requirements of JIS G4303/G4304 for SUS304H with ASTM A240 for UNS S30409.
| Element | SUS304H, JIS G4303/G4304, wt % | ASTM A240 304H, wt % |
|---|---|---|
| Carbon, C | 0.04 - 0.10 | 0.04 - 0.10 |
| Silicon, Si | 1.00 max | 0.75 max |
| Manganese, Mn | 2.00 max | 2.00 max |
| Phosphorus, P | 0.045 max | 0.045 max |
| Sulfur, S | 0.030 max | 0.030 max |
| Chromium, Cr | 18.00 - 20.00 | 18.0 - 20.0 |
| Nickel, Ni | 8.00 - 10.50 | 8.0 - 10.5 |
| Iron, Fe | Balance | Balance |
Mechanical Properties
In the solution-annealed condition, SUS304H shall meet the following room-temperature requirements per JIS G4303 and G4304. The ASTM A240 values for 304H are equivalent within rounding.
| Property | JIS G4303/G4304 SUS304H | ASTM A240 304H |
|---|---|---|
| Tensile strength | 520 MPa min | 515 MPa min |
| Yield strength, 0.2 % offset | 205 MPa min | 205 MPa min |
| Elongation | 40 % min | 40 % min |
Because of the higher carbon content, SUS304H should not be used at cryogenic temperatures; the low-carbon grades SUS304L are the correct choice when low-temperature toughness is the governing requirement.
High-Temperature Behavior
The value of SUS304H appears only above roughly 500 °C, where standard 304 creeps too quickly under sustained load:
Creep resistance: carbon atoms pin grain boundaries and slow dislocation climb, so the grade holds dimensional stability under constant load in the 500 to 800 °C range.
Oxidation resistance: the chromium-rich oxide scale protects the surface in air and steam up to about 870 °C continuous service. Short-term exposure to approximately 925 °C is possible but shortens service life.
Design limits: pressure design codes such as ASME Section VIII and B31.3 limit design stresses for 304H to roughly 816 °C. Above 900 °C, the austenite structure becomes unstable and strength drops sharply, and higher-alloy grades such as 310S should be selected.
Sigma-phase caution: prolonged service in the 600 to 900 °C range can promote sigma-phase formation, which reduces ductility; design life and inspection intervals should account for this.
Welding and Fabrication
Filler metal: ER308H per AWS A5.9 matches the carbon level of the base metal and is preferred for high-temperature design. Low-carbon ER308L reduces weld creep strength.
Heat input: moderate heat input with controlled interpass temperature limits carbide precipitation in the heat-affected zone.
Heat treatment: the grade is used in the solution-annealed condition, 1010 to 1120 °C followed by rapid cooling. Post-weld heat treatment is generally not required for high-temperature service.
Inspection: for boiler and pressure parts, non-destructive testing is normally required by the governing code to confirm weld soundness.
Comparing SUS304H with Related Grades
| Grade | Best for | Limitation |
|---|---|---|
| SUS304 | General room-temperature and mild service | No guaranteed creep strength above 500 °C |
| SUS304H | High-temperature air and steam, creep-loaded parts | Poor low-temperature toughness, sensitization risk when welded |
| SUS316H | High temperature plus chloride or sulfur corrosion | Higher alloy cost than 304H |
| SUS310S | Above 900 °C, strongly oxidizing service | Highest cost of the four, thermal-fatigue sensitivity |
Typical Applications
Boiler superheater and reheater tubes
High-temperature process piping and manifolds
Furnace parts, radiant tubes and heat-treatment fixtures
Heat-exchanger tubes in power and process plants
Chemical reactor internals in non-corrosive high-temperature service
Frequently Asked Questions
Q1. Why is SUS304H suitable for high-temperature applications?
The controlled carbon range of 0.04 to 0.10 percent provides creep strength through solid-solution and carbide strengthening. At 500 to 800 °C, standard SUS304 creeps under sustained load while SUS304H maintains its shape, and the chromium oxide scale resists oxidation in air and steam.
Q2. Is EN 1.4307 equivalent to SUS304H?
No. EN 1.4307 (X2CrNi18-9) is the European designation for 304L, the low-carbon grade with 0.030 percent maximum carbon. SUS304H is the high-carbon grade; EN 10088-2 has no direct 304H listing, so ASTM TP304H is normally specified for this chemistry in European projects.
Q3. What is the maximum operating temperature of SUS304H?
Continuous service is practical to about 870 °C in air and steam, with short-term exposure to about 925 °C possible at the cost of reduced life. Pressure design codes limit design stresses to roughly 816 °C, and above 900 °C higher-alloy grades such as 310S are required.
Q4. How do you avoid problems when welding SUS304H?
Use ER308H filler to match the carbon level, control heat input and interpass temperature, and avoid unnecessary multi-pass reheating. Post-weld solution annealing at 1010 to 1120 °C with rapid cooling restores corrosion resistance if required.
Q5. Can SUS304H be used at low temperature?
It is not recommended. The higher carbon content reduces low-temperature toughness, and below about -40 °C the grade can become brittle under impact. SUS304L is the correct choice for cryogenic service.
Q6. What is the difference between SUS304H and SUS316H?
SUS316H adds 2 to 3 percent molybdenum, giving much better resistance to chloride and sulfur attack in high-temperature corrosive environments, at a higher alloy cost. SUS304H is the cost-effective choice for hot, non-aggressive atmospheres such as air and steam.