EN Grades 1.4404, 1.4462, 1.4539 Corrosion Ranking

Apr 15, 2026

Leave a message

Quick answer: ranked by PREN alone, 1.4462 (about 35) and 1.4539 (about 34) are effectively tied and both sit far above 1.4404 (about 25). Ranked by chloride pitting temperature, 1.4462 leads. Ranked by acid resistance, 1.4539 leads outright. Ranked by stress corrosion cracking, 1.4462 leads. Ranked by cost, the order reverses completely. There is no single ranking - the order changes with the medium, which is the point of this page.

1. Basic Definition and Metallurgical Characteristics

1.1 1.4404 (316L): the baseline

1.4404 is austenitic 316L: Cr 16.0-18.0%, Ni 10.0-14.0%, Mo 2.00-3.00%, C 0.030% maximum, PREN about 25. It defines the entry level for chloride-bearing service and is the reference against which the other two are measured.

1.2 1.4462 (2205 duplex): the chloride specialist

1.4462 adds chromium to 21-23%, molybdenum to 3.0-3.5% and nitrogen to 0.14-0.20%, and changes structure to roughly 50% ferrite. PREN rises to about 35 and yield to 450 MPa. Its ranking advantage is concentrated in chloride pitting and stress corrosion cracking, not in acid.

1.3 1.4539 (904L): the acid specialist

1.4539 raises nickel to 24-26%, molybdenum to 4.0-5.0% and adds 1.2-2.0% copper, with carbon at 0.020% maximum. PREN is about 34 - marginally below 2205 - yet its performance in sulphuric and phosphoric acid is in a different class, because nickel and copper govern there, not PREN.

2. Core Parameter Comparison

2.1 Chemical composition (wt%, ASTM A240)

Element 1.4404 1.4462 1.4539 What it drives
Cr 16.0-18.0 21.0-23.0 19.0-23.0 Passive film strength
Ni 10.0-14.0 4.5-6.5 24.0-26.0 Acid resistance and austenite stability
Mo 2.00-3.00 3.0-3.5 4.0-5.0 Chloride pitting
N 0.10 max 0.14-0.20 0.10 max Strength and PREN in duplex
Cu - - 1.20-2.00 Sulphuric acid resistance
C 0.030 max 0.030 max 0.020 max Weld sensitisation
PREN about 25 about 35 about 34 Pitting index only

The table already shows the trap: 1.4539 has the lowest chromium of the two high grades and a PREN below 2205, yet it is the most corrosion resistant in acid. Any ranking built purely on PREN will mislead exactly where the money is highest.

2.2 Mechanical properties (which affect ranking indirectly)

Property 1.4404 1.4462 1.4539
Yield strength (0.2%) 170 MPa min 450 MPa min 220 MPa min
Tensile strength 485 MPa min 620 MPa min 490 MPa min
Elongation 40% 25% 35%
Max service temperature about 870 C about 300 C about 400 C
Relative metal price 1.00 0.92-1.05 2.05-2.40

2.3 Ranking table by mechanism

Read this as five separate rankings, not one ladder.

Mechanism 1st 2nd 3rd Governing factor
Chloride pitting, ambient 1.4462 1.4539 1.4404 PREN, with duplex ahead on CPT
Critical pitting temperature, 1 M NaCl 1.4462 (50-55 C) 1.4539 (45-50 C) 1.4404 (20-25 C) Nitrogen plus phase structure
Chloride SCC above 60 C 1.4462 1.4539 (marginal) 1.4404 (poor) Ferrite interrupts cracking
Sulphuric acid, dilute 1.4539 1.4462 (poor) 1.4404 (fails) Nickel plus copper
Phosphoric acid 1.4539 1.4462 (limited) 1.4404 (fails) Copper
Seawater, high velocity 1.4462 1.4539 1.4404 Hardness and PREN
Seawater, stagnant None adequate - - Requires 6Mo or super duplex
Cost (lowest first) 1.4404 1.4462 1.4539 Nickel content
High temperature use 1.4404 (870 C) 1.4539 (400 C) 1.4462 (300 C) Sigma and phase stability

Notice the reversals: 1.4462 is first on four rows and last on two; 1.4539 is first on three rows but most expensive by a wide margin. Any page that presents a single ordered list is either simplifying for marketing or simply wrong.

2.4 Welding and fabrication (a practical ranking dimension)

Item 1.4404 1.4462 1.4539
WPS complexity Simple Controlled heat input Moderate, purge critical
Interpass limit 250 C 150 C 250 C
Filler availability Universal Wide Limited and costly
Post-weld anneal Not needed Sometimes Not needed
Machining difficulty Moderate High Very high
Site repairability Good Poor Moderate

2.5 Price ranking and cost per year of life

Indicative FOB China, USD per tonne, plate 4-12 mm, 2-10 t.

Grade Price (USD/t) Relative Typical life in 500 mg/l chloride at 60 C
1.4404 3,150-3,550 1.00 2-5 years
1.4462 2,850-3,300 0.92-1.05 15-25 years
1.4539 6,300-8,300 2.05-2.40 10-15 years (chloride) / 10-20 years (acid)

In that specific duty, the cheapest metal delivers the longest life - which is why ranking by price per tonne and ranking by fitness are unrelated exercises.

3. Applicable Duty and Selection Guide

3.1 Duty map for each grade

1.4404: neutral chloride up to about 500 mg/l, food and pharma, general chemical, cooling water, architectural exteriors away from surf

1.4462: seawater and brine with flow, desalination, FGD, chlorinated cooling water, pressure vessels where strength reduces wall

1.4539: sulphuric and phosphoric acid, leach circuits, acid storage, scrubber liquors with acid condensation

3.2 Ranking by severity, not by grade

Severity band Medium Recommended grade Next step up
1 - mild Potable water, indoor atmosphere 1.4301 / 1.4404 1.4404
2 - moderate Chloride 200-500 mg/l, coastal air 1.4404 1.4462
3 - severe chloride Seawater, brine, chlorinated water 1.4462 Super duplex
4 - acid Dilute sulphuric or phosphoric acid 1.4539 Nickel alloy
5 - mixed Acid plus chloride plus temperature 1.4539 or nickel alloy Alloy 20 / C276

3.3 Three-step selection test

Step Question If yes If no
1. Acid pH below 3 or sulphuric/phosphoric acid present? 1.4539, ranked first on acid Continue
2. Chloride plus heat Chloride with temperature above 60 C? 1.4462, ranked first on SCC Continue
3. Temperature ceiling Service above 300 C? 1.4404 only; duplex is out Compare cost

4. What We Supply for All Three Grades

20+ years of manufacturing, 50+ export markets, 200+ energy and petrochemical projects delivered.

Product 1.4404 1.4462 1.4539 Standard
Plate 3.0-80 mm 3.0-60 mm 3.0-50 mm A240
Sheet 0.3-3.0 mm 0.4-3.0 mm 0.5-3.0 mm A240
Seamless tube 6-219 mm 6-219 mm 6-219 mm A213
Bar 10-300 mm 10-300 mm 10-250 mm A276
Fittings DN15-DN600 DN15-DN600 DN15-DN300 A403 / A815

Every order ships with PREN calculated from the actual heat analysis, plus the grade-specific evidence each one needs: nitrogen and ferrite for 1.4462, copper and nickel for 1.4539, carbon and molybdenum for 1.4404.

Send the medium, concentration, temperature and chloride level - we will rank the three grades for your specific duty and show the cost of each, rather than quoting a default. If your duty falls in band 4 or 5, say acid at enquiry: it changes the ranking before any price discussion.

5. FAQ: Corrosion Ranking of 1.4404, 1.4462 and 1.4539

Which of the three is the most corrosion resistant?

There is no single answer. In chloride 1.4462 ranks first; in acid 1.4539 ranks first by a wide margin; in hot chloride with stress 1.4462 wins; above 300 C only 1.4404 remains usable. The correct question is which medium, at what concentration and temperature.

Is 904L better than 2205 because it costs more?

No. 1.4539 has PREN about 34 against 35 for 1.4462, lower yield strength and roughly 2.2 times the price. It is 'better' only in acid service. In seawater, 2205 outperforms it at a fraction of the cost - paying more does not buy a higher ranking in every medium.

Why does the ranking change above 300 C?

Because duplex grades form sigma phase in long service above about 300 C, losing toughness and corrosion resistance, while austenitic grades do not. At 400 C the duplex advantage disappears entirely and 1.4404 becomes the only sensible choice among the three.

What PREN should I require for seawater?

For ambient flowing seawater, PREN 34-36 is the practical minimum, which points to 2205 or 904L. For chlorinated or warm seawater, PREN 40 or above is required, which means super duplex or 6Mo. Below PREN 30, seawater service is not defensible regardless of the grade name.

Does higher PREN always mean longer life?

No. PREN predicts pitting resistance in chloride only. In acid, in crevices, in erosion or under deposits the governing factors are nickel, copper, geometry, velocity and surface finish. A higher PREN number can hide a weaker performance in the actual medium - which is the central lesson of this comparison.

Can I use one grade for a plant with mixed duties?

Sometimes: 1.4539 covers mild acid plus chloride and is the most versatile of the three, at the highest cost. But using one grade everywhere usually means over-paying on most lines and under-performing on the worst one. A line-by-line duty map normally pays for itself within the first procurement cycle.

Which grade is easiest to fabricate?

1.4404, clearly: widest filler availability, most tolerant welding window, easiest machining and best site repairability. 1.4462 requires a controlled WPS and hard machining; 1.4539 requires a purged weld and expensive filler. Fabrication capability is a genuine ranking dimension that price lists ignore.

What data should I demand to justify the ranking?

PREN from the actual analysis, critical pitting temperature test data where the duty is chloride, corrosion rate data for the specific acid concentration and temperature, and the welding procedure. Marketing claims about 'superior corrosion resistance' without medium-specific data are not evidence.

Applications of Type 410 Stainless Steel
Hardenable Martensitic Stainless Steel: Grade 4101.4006 in China
Grade 416 Stainless Steel
Grade 409 (UNS S40900) in China

Send Inquiry