EN 1.4401 Stainless Steel: Composition, Properties and Grades

Apr 08, 2026

Leave a message

What EN 1.4401 Actually Specifies

EN 1.4401 is the material number for the austenitic stainless steel designated X5CrNiMo17-12-2 in the European standard system. It is the European counterpart of AISI 316 and UNS S31600: a chromium-nickel-molybdenum austenitic grade with roughly 17% chromium, 10-13% nickel and 2.0-2.5% molybdenum. Searches for "EN 1.4401 stainless steel PDF" usually mean the mill datasheet, and the technical content of that datasheet is defined by EN 10088-1 for composition and by the relevant product standard for mechanical properties and tolerances. The molybdenum addition is the defining feature of the grade: it substantially improves resistance to pitting and crevice corrosion in chloride-bearing and acidic environments compared with the molybdenum-free 304 family, which is why 1.4401 remains a standard choice for process equipment, architectural fabrications and general corrosion service.

Chemical Composition to EN 10088-1

Element Content (%)
Carbon (C) ≤ 0.07
Silicon (Si) ≤ 1.00
Manganese (Mn) ≤ 2.00
Phosphorus (P) ≤ 0.045
Sulfur (S) ≤ 0.015
Chromium (Cr) 16.5-18.5
Nickel (Ni) 10.0-13.0
Molybdenum (Mo) 2.00-2.50
Nitrogen (N) ≤ 0.10

The corresponding pitting resistance equivalent number is about 24-25, calculated as Cr + 3.3 Mo + 16 N, which places 1.4401 clearly above the molybdenum-free 304 grades but well below molybdenum-rich or duplex alternatives used for aggressive chloride service.

Mechanical and Physical Properties

Properties below refer to the annealed condition; cold-worked bar and wire are supplied to higher strength levels under their own product standards.

Property Typical value
Tensile strength, Rm 500-700 MPa
0.2% proof strength, Rp0.2 ≥ 200 MPa
Elongation, A ≥ 40%
Hardness ≤ 215 HB
Modulus of elasticity 200 GPa
Density 8.0 g/cm³
Thermal conductivity at 20 °C about 15 W/m·K
Electrical resistivity at 20 °C about 0.75 µΩ·m
Service temperature range -196 °C to 550 °C

In the annealed condition 1.4401 is essentially non-magnetic, with a relative permeability close to 1.02, but cold working such as bending, drawing or machining can generate a small amount of ferromagnetic martensite. Where a very low permeability is required, the part must be annealed after forming or specified as a low-ferrite variant.

Product Forms and Delivery Standards

A complete purchase specification for 1.4401 names both the grade and the product standard, because composition is fixed by EN 10088-1 while dimensions, tolerances and mechanical requirements come from the form standard.

Flat products: EN 10088-2 for sheet, plate and strip, with EN 10028-7 for pressure-vessel plate.

Long products: EN 10088-3 for bar, rod and sections, and EN 10088-5 for wire rod.

Tube and pipe: EN 10216-5 for seamless tube, EN 10217-7 for welded tube, and equivalent ASTM A312 and A213 for projects that follow US practice.

Forgings and castings: EN 10222-5 for forgings, with matching filler and welding consumables to the appropriate consumable standard.

Certification: inspection documents to EN 10204 type 3.1 as standard, with 3.2 available when third-party witnessing is required; product analysis, tensile testing and intergranular corrosion testing to EN ISO 3651-2 can be added.

Selecting Between 1.4401 and Its Close Variants

The main selection decision is carbon content and molybdenum level, since four grades in the same family cover most of the applications where 1.4401 is considered.

1.4401 (316): carbon ≤ 0.07%. Good general corrosion resistance and adequate for thin-section welded parts and machined components.

1.4404 (316L): carbon ≤ 0.03%. Lower carbon limits sensitisation and intergranular corrosion after welding, so it is preferred for welded pressure vessels, heavy sections and sanitary pipelines.

1.4432 and 1.4435: higher molybdenum at 2.5-3.0%, with 1.4435 also controlled for low ferrite content, which is why it is used for pharmaceutical and hygienic process equipment where both corrosion resistance and phase purity matter.

1.4571 (316Ti): titanium-stabilised for elevated-temperature service where carbon precipitation must be prevented over long exposure.

Service limits should be stated explicitly in the specification. 1.4401 performs well in atmospheric exposure, fresh water, mild acids and brackish water, but long-term exposure to warm, high-chloride seawater is a different duty, where duplex grades offer a much larger safety margin. It is also susceptible to chloride stress corrosion cracking above roughly 60 °C in concentrated chloride conditions, and to intergranular attack if sensitised material is placed in service after welding. For pressure equipment in Europe, compliance with the Pressure Equipment Directive and with the associated material specifications, such as the AD 2000 material data sheets, is normally part of the qualification.

FAQ: EN 1.4401 in Service

Q: What is the difference between EN 1.4401 and 1.4404?
Only the carbon range differs in practical terms: 1.4401 allows up to 0.07% carbon while 1.4404 is limited to 0.03%, which makes 1.4404 the better choice for welded heavy sections.

Q: Is EN 1.4401 suitable for seawater service?
It resists brackish and mildly salty water, but for continuous high-chloride seawater at elevated temperature a duplex grade such as 1.4462 provides a far larger pitting and crevice corrosion margin.

Q: Is EN 1.4401 magnetic?
In the annealed condition it is essentially non-magnetic, but cold working can produce slight magnetism, which can be removed by annealing if a low permeability is required.

Q: Can EN 1.4401 be used for food and pharmaceutical equipment?
Yes, provided the surface finish and welding controls suit the duty; for welded product-contact equipment the low-carbon 1.4404 or the low-ferrite 1.4435 is usually preferred.

Q: How is EN 1.4401 welded?
It welds readily by TIG, MIG and manual metal arc processes using matching 316L filler, with no preheat and normally no post-weld heat treatment; the low-carbon variant is chosen when the joint is thick or restraint is high.

Q: Which certificates should be requested with an EN 1.4401 order?
An EN 10204 type 3.1 inspection certificate as a minimum, with product analysis and intergranular corrosion testing added for pressure and process applications.