1.4404 vs 1.4571: 316L vs 316Ti Stainless Steel
Apr 15, 2026
Leave a message
Quick answer: 1.4404 and 1.4571 are both 316-family stainless steels with 2-3% molybdenum and the same PREN of about 25. The difference is how each handles carbon: 1.4404 keeps carbon at 0.030% maximum so carbides cannot form, while 1.4571 allows up to 0.08% carbon and adds titanium at five times the carbon content to tie it up. Neither resists chloride better. 1.4571 wins only where the part is welded in heavy section or held between 450 and 900 C.
1. Basic Definition and Metallurgical Characteristics
1.1 1.4404 (316L): low carbon, no stabiliser
1.4404, AISI 316L, UNS S31603, holds carbon at 0.030% maximum with Cr 16.0-18.0%, Ni 10.0-14.0% and Mo 2.00-3.00%. The low carbon is the whole protection strategy: with so little carbon available, chromium carbides cannot precipitate at grain boundaries even after welding, so the heat-affected zone keeps its chromium in solution and therefore keeps its corrosion resistance.
The limit of this approach is real and often ignored: carbon is not zero, and at large section thickness the cooling rate through the 450-850 C sensitisation range is slow enough that even 0.030% carbon can form enough carbide to matter. That is why heavy-section vessels sometimes specify a stabilised grade instead.
1.2 1.4571 (316Ti): titanium stabilised
1.4571, AISI 316Ti, UNS S31635, permits carbon up to 0.08% and requires titanium between five times the carbon content and 0.70%. Titanium has a stronger affinity for carbon than chromium does, so it forms titanium carbides during solidification and high-temperature exposure, leaving chromium free to maintain the passive film. The grade is therefore immune to sensitisation regardless of section thickness or cooling rate.
Its limits: titanium additions can produce titanium nitride and carbonitride inclusions that slightly reduce polishability and weld cleanliness; the grade is harder to obtain in thin sheet than 1.4404; and it does nothing for chloride pitting beyond what the molybdenum already provides.
2. Core Parameter Comparison
2.1 Chemical composition (wt%, ASTM A240 / EN 10088-2)
| Element | 1.4404 spec | 1.4404 typical | 1.4571 spec | 1.4571 typical | Design intent |
|---|---|---|---|---|---|
| C | 0.030 max | 0.019 | 0.08 max | 0.048 | Carbon strategy divides the grades |
| Ti | - | - | 5 x C to 0.70 | 0.35 | Ties carbon, prevents carbide at grain boundaries |
| Cr | 16.0-18.0 | 16.9 | 16.0-18.0 | 16.8 | Identical range and function |
| Ni | 10.0-14.0 | 10.3 | 10.0-14.0 | 10.5 | Same austenite stability |
| Mo | 2.00-3.00 | 2.10 | 2.00-3.00 | 2.12 | Same PREN contribution |
| Mn | 2.00 max | 1.25 | 2.00 max | 1.28 | Substitution indicator |
| Si | 0.75 max | 0.40 | 0.75 max | 0.42 | Slag control in welding |
| P | 0.045 max | 0.028 | 0.045 max | 0.029 | Cracking sensitivity |
| S | 0.030 max | 0.001 | 0.030 max | 0.001 | Pit initiation sites |
| N | 0.10 max | 0.040 | 0.10 max | 0.038 | Small PREN contribution |
Check the titanium ratio, not just the presence. With 0.048% carbon the minimum titanium is 0.24%; a certificate showing 0.15% titanium against 0.05% carbon is out of specification even though it says "316Ti". The stoichiometric requirement is Ti:C of at least 4:1, and the standard demands 5:1 for margin.
2.2 Room-temperature mechanical properties
| Property | 1.4404 min | 1.4404 typical | 1.4571 min | 1.4571 typical |
|---|---|---|---|---|
| Tensile strength | 485 MPa | 580-670 MPa | 515 MPa | 590-680 MPa |
| Yield strength (0.2%) | 170 MPa | 245-300 MPa | 205 MPa | 255-320 MPa |
| Elongation | 40% | 46-55% | 40% | 45-54% |
| Hardness | 217 HBW max | 160-185 HB | 217 HBW max | 165-190 HB |
| Elevated strength at 600 C | Low | about 120 MPa 0.2% | Low | about 135 MPa 0.2% |
The minimum values in 1.4571 are slightly higher only because the grade is specified against a different table; delivered values overlap. Selection on mechanical grounds is not meaningful here - both are austenitic, neither hardens by heat treatment, and both lose roughly half their strength by 600 C.
2.3 Corrosion resistance and sensitisation behaviour
PREN = Cr + 3.3 x Mo + 16 x N = about 24.9 for both grades. The comparison below is therefore not about pitting - it is about the heat-affected zone.
| Condition | 1.4404 | 1.4571 | Mechanism |
|---|---|---|---|
| Pitting resistance, ambient | about 500 mg/l chloride | about 500 mg/l chloride | Identical Mo level |
| Chloride SCC above 60 C | Risk | Risk | Ti does not prevent SCC |
| Weld HAZ, 3 mm sheet | Safe | Safe | Both fine at thin gauge |
| Weld HAZ, 12 mm plate | Marginal without control | Safe | Slow cooling plus carbon |
| Hold 450-850 C, 100 h | Sensitisation possible | No sensitisation | Ti stabilisation at work |
| Post-weld stress relief 600 C | Risk of sensitisation | Safe | The decisive fabrication case |
| Repeated weld repair | Each pass adds risk | Tolerant | Repair is where Ti earns its cost |
| Sigma phase 500-800 C | Forms over long hold | Forms equally | Ti does not prevent sigma |
The last row matters because it is frequently misunderstood: titanium suppresses carbide precipitation, not sigma phase. A 316Ti part held at 700 C for thousands of hours still embrittles and still loses toughness. Stabilisation solves one problem, not all high-temperature problems.
2.4 Welding, machining and forming
| Item | 1.4404 | 1.4571 | Practice |
|---|---|---|---|
| Filler metal | ER316L | ER316Ti or ER316L acceptable | Matching filler keeps Ti in the weld |
| Post-weld heat treatment | Avoid 450-850 C unless required | Stress relief at 600 C is safe | Ti is why stabilised grades exist |
| Heat input | Normal, 1-3 kJ/mm | Normal, but avoid long dwell | Neither needs duplex-style control |
| Machining | Gummy, work-hardens | Slightly abrasive due to Ti inclusions | Expect 5-10% more tool wear |
| Deep drawing | Excellent | Good, marginally lower ductility | 1.4404 preferred for severe draws |
| Polishing | Good response | Slight inclusion pull-out | 1.4404 for 8K mirror work |
| Weld repair on site | Procedure needed | More forgiving | The reason refineries specify 316Ti |
2.5 Price and lifecycle cost
Indicative FOB China, USD per tonne, plate 4-12 mm, 3-15 t lot.
| Item | 1.4404 | 1.4571 | Comment |
|---|---|---|---|
| Metal price (indicative) | 3,150-3,550 | 3,250-3,650 | Ti adds 3-8% |
| Availability in thin sheet | Universal | Limited below 2 mm | Affects lead time, not just price |
| Welding cost | Baseline | Baseline, less rework | Rework on thick 316L is expensive |
| Life, thin sheet, normal welds | 20+ years | 20+ years | No difference |
| Life, thick welded vessel at 600 C | HAZ attack within years | 15-25 years | The payback case |
Rule: below 6 mm with normal welding, 1.4571's premium buys nothing. Above 10 mm, or wherever a 600 C stress relief is specified, it buys the whole service life of the part.
3. Applicable Duty and Selection Guide
3.1 Where 1.4404 is the right choice
Sheet and thin-plate fabrication below 6 mm
Architectural, catering and medical equipment surfaces
Mirror and brushed finishes where inclusion-free polish matters
Dairy, brewery and pharmaceutical lines with full CIP rinse
General chemical plant pipework with dilute chloride
Any part where 1.4571 is unavailable in the required gauge
3.2 Where 1.4571 is the right choice
Pressure vessels and reactors above 10 mm wall
Equipment that receives post-weld stress relief at 550-650 C
Reformer and furnace internals cycling through 450-900 C
Heat exchanger tube sheets and thick flanges
Refinery and petrochemical lines where weld repair is expected
Components welded repeatedly during manufacture or maintenance
Flue-gas and exhaust sections below 900 C with condensation risk
3.3 Three-step selection test
| Step | Question | If yes | If no |
|---|---|---|---|
| 1. Section | Wall above 10 mm, or multipass welding? | Consider 1.4571 | 1.4404 is sufficient |
| 2. Thermal | Stress relief at 550-650 C, or service 450-850 C? | 1.4571 mandatory | Continue to step 3 |
| 3. Repair | Will the part be weld repaired in service? | 1.4571 reduces risk | 1.4404, lower cost |
4. What We Supply for Both Grades
20+ years of manufacturing, 50+ export markets, 200+ energy and petrochemical projects delivered.
| Product | 1.4404 | 1.4571 | Standard |
|---|---|---|---|
| Cold-rolled sheet | 0.3-3.0 mm | 1.0-3.0 mm | A240 / EN 10088-2 |
| Hot-rolled plate | 3.0-80 mm | 3.0-60 mm | A240 / EN 10028-7 |
| Coil and strip | 0.3-6.0 mm | 2.0-6.0 mm | A240 / A480 |
| Seamless tube | 6-219 mm | 6-219 mm | A213 / A269 |
| Bar | 10-300 mm | 10-300 mm | A276 / A479 |
1.4571 certificates report titanium as a number alongside carbon, so the 5:1 ratio can be verified without calculation. PMI, impact testing and third-party inspection available on request.
Send the wall thickness, welding procedure and any stress-relief temperature - we will tell you whether 1.4571 is necessary or whether 1.4404 saves you 3-8% for the same service life. If your specification already names 316Ti, we will confirm the titanium ratio from the heat analysis before shipment.
5. FAQ: 1.4404 vs 1.4571
Is 316Ti more corrosion resistant than 316L?
No, at least not in pitting or general corrosion: both have 2-3% molybdenum and the same PREN of about 25. 316Ti is more resistant only to intergranular corrosion after welding or elevated-temperature exposure, because titanium prevents chromium carbide precipitation. Marketing that presents 316Ti as a higher corrosion class is technically wrong.
Why does 316Ti exist if 316L is cheaper?
Because low carbon has a thickness limit. At large section sizes the cooling rate through the sensitisation range is slow enough that 0.030% carbon still forms carbides, and because many processes require a 600 C stress relief that would sensitise 316L outright. Titanium removes both constraints, at the cost of about 3-8%.
Can 316L be stress relieved?
Only with care. Stress relief at 550-650 C puts 316L directly in the sensitisation range, so a subsequent pickle and passivate is essential, and thick sections may still lose HAZ corrosion resistance. If the design requires stress relief, specify 316Ti or 316H rather than accepting the risk.
Does titanium prevent sigma phase?
No. Sigma phase forms in the 500-800 C range in all molybdenum-bearing austenitic grades, including 316Ti, and it embrittles the steel over thousands of hours. Titanium addresses carbide precipitation only. Long-service 316Ti parts above 600 C still need a fitness-for-service assessment.
Can I use 316L filler on 316Ti?
Yes, and it is common: ER316L diluted with the 316Ti base metal gives a weld with adequate titanium from dilution and low carbon from the filler. For critical high-temperature welds, ER316Ti is preferred so the deposit itself is stabilised.
Are the two grades interchangeable in a specification?
Only in one direction safely: if a specification calls for 316Ti, substituting 316L is a downgrade for thick-section or stress-relieved service and requires client approval. If it calls for 316L, 316Ti is generally acceptable as an upgrade, though it may not be listed in the applicable code table.
Which is better for chloride?
Identical. Chloride pitting depends on molybdenum, chromium and nitrogen, all of which are the same. If the problem is chloride, neither grade is an upgrade over the other - the answer is 6Mo, duplex or super duplex. Choosing 316Ti for "better chloride resistance" is a common and expensive misunderstanding.
What documents verify titanium stabilisation?
The MTR must report both carbon and titanium so the 5:1 ratio can be checked, plus PMI on the finished part. A certificate that states "stabilised" without numbers proves nothing. We report Ti and C numerically on every 1.4571 heat and flag any heat below 5:1 before shipment.



Send Inquiry