1.4404 vs 1.4462 Duplex Steel: PREN & Application
Apr 15, 2026
Leave a message
1.1 1.4404 (316L): single-phase austenite
1.4404, AISI 316L, UNS S31603, is a fully austenitic chromium-nickel-molybdenum stainless steel: Cr 16.0-18.0%, Ni 10.0-14.0%, Mo 2.00-3.00%, C 0.030% maximum. Its face-centred cubic structure gives high toughness at any temperature, excellent formability, and near-isotropic behaviour. Strength comes only from cold work; heat treatment can soften but never harden it. The low carbon prevents sensitisation during welding, and molybdenum gives chloride tolerance up to roughly 500 mg/l at ambient.
1.2 1.4462 (2205 duplex): ferrite plus austenite
1.4462, UNS S32205 (also S31803 in older specifications), is a duplex stainless steel with roughly equal proportions of ferrite and austenite: Cr 21.0-23.0%, Ni 4.5-6.5%, Mo 3.0-3.5%, N 0.14-0.20%, C 0.030% maximum. The two-phase structure delivers about twice the yield strength of austenitic grades, immunity to chloride stress corrosion cracking in the temperature range where 316L cracks, and better resistance to erosion-corrosion because of its higher hardness.
The trade-off is metallurgical: the balanced structure is only correct if the thermal history is correct. Welding above roughly 150 C interpass, or slow cooling through 700-950 C, precipitates sigma phase and brittle intermetallic phases that destroy toughness and corrosion resistance. Duplex is therefore a material for fabricators with a qualified welding procedure, not for site improvisation.
2. Core Parameter Comparison
2.1 Chemical composition (wt%, ASTM A240 / EN 10088-2)
| Element | 1.4404 spec | 1.4404 typical | 1.4462 spec | 1.4462 typical | Function in duplex |
|---|---|---|---|---|---|
| C | 0.030 max | 0.019 | 0.030 max | 0.020 | Above 0.03 harms phase balance |
| Cr | 16.0-18.0 | 16.9 | 21.0-23.0 | 22.3 | Five points more Cr is the base of duplex resistance |
| Ni | 10.0-14.0 | 10.3 | 4.5-6.5 | 5.6 | Lower Ni plus N balances the ferrite |
| Mo | 2.00-3.00 | 2.10 | 3.0-3.5 | 3.2 | Raises PREN and pitting resistance |
| N | 0.10 max | 0.040 | 0.14-0.20 | 0.17 | Strength, austenite formation, PREN |
| Mn | 2.00 max | 1.25 | 2.00 max | 1.20 | Substitution check |
| Si | 0.75 max | 0.40 | 1.00 max | 0.45 | Above 1% promotes sigma |
| P | 0.045 max | 0.028 | 0.030 max | 0.022 | Duplex limit is tighter |
| S | 0.030 max | 0.001 | 0.020 max | 0.001 | Tighter limit for weld quality |
Two numbers deserve attention. Duplex nitrogen at 0.14-0.20% is a specification requirement, not an aim: it contributes about 2.4 PREN points and it is what restores austenite after welding. A duplex certificate showing 0.10% N is out of specification, and that is the single most common duplex substitution we are asked to inspect.
2.2 Room-temperature mechanical properties
| Property | 1.4404 min | 1.4404 typical | 1.4462 min | 1.4462 typical | Design consequence |
|---|---|---|---|---|---|
| Yield strength (0.2%) | 170 MPa | 245-300 MPa | 450 MPa | 480-550 MPa | Duplex allows thinner walls |
| Tensile strength | 485 MPa | 580-670 MPa | 620 MPa | 700-800 MPa | Higher burst margin |
| Elongation | 40% | 46-55% | 25% | 28-33% | Less formability; more springback |
| Hardness | 217 HBW max | 160-185 HB | 290 HBW max | 240-270 HB | Better erosion resistance; harder to machine |
| Impact at -46 C | High, no transition | 100+ J | Limited by ferrite | 27 J min typical requirement | Duplex needs impact testing |
| Max service temperature | about 870 C (oxidation limit) | - | about 300 C practical | - | Sigma above 300 C in long service |
The wall-thickness consequence is the commercial core of this comparison. In a pressure application limited by yield, going from 170 MPa to 450 MPa allows roughly a 60% reduction in required thickness. A 10 mm 316L shell can often become 6 mm duplex for the same design pressure - which means about 40% less metal, and often a lower total cost despite a higher price per tonne.
2.3 Corrosion resistance and PREN
PREN = Cr + 3.3 x Mo + 16 x N.
| Index / mechanism | 1.4404 | 1.4462 | Engineering meaning |
|---|---|---|---|
| PREN (typical) | about 24.9 | about 35.4 | Duplex is 1.4x in pitting resistance |
| Critical pitting temperature, 1 M NaCl | about 20-25 C | about 50-55 C | The temperature where pits start |
| Chloride SCC | Risk above 60 C | Largely immune below 150 C | The main reason duplex is chosen |
| Chloride limit, ambient, flowing | about 500 mg/l | Seawater acceptable with velocity above 1 m/s | Duplex is a seawater-grade material |
| Stagnant seawater | Fails | Marginal - crevice and biofouling risk | Neither likes stagnant seawater |
| Dilute sulphuric acid | Limited | Limited, no Cu | Neither is a sulphuric-acid alloy |
| Erosion-corrosion | Moderate | Good | Hardness nearly doubles |
| Above 300 C long service | Acceptable to 870 C | Sigma precipitation, toughness loss | The hard limit of duplex |
Read the last two rows as a pair: duplex is far better where the problem is chloride, and far worse where the problem is heat. A 2205 part in a 400 C flue-gas line will embrittle regardless of how good its PREN looks on paper.
2.4 Welding, machining and forming
| Item | 1.4404 | 1.4462 | Rule of practice |
|---|---|---|---|
| Heat input | Wide window, 1-3 kJ/mm acceptable | 0.5-2.0 kJ/mm, controlled | Duplex needs a written WPS |
| Interpass temperature | Up to 250 C tolerable | 150 C maximum | Measure it, do not estimate |
| Filler metal | 316L (ER316L) | ER2209, over-alloyed | Matching composition preserves balance |
| Post-weld heat treatment | None required | Solution anneal at 1,050-1,100 C if balance is lost | PWHT is not a routine option |
| Machining | Gummy, work-hardening | Harder, 20-30% higher cutting force | Duplex needs carbide tooling, lower speed |
| Forming | Excellent, 40% elongation | 25% elongation, high springback | Duplex cold forming limited to mild shapes |
| Heat tint after welding | Pickle and passivate | Pickle and passivate; oxide is a corrosion site here too | Never skip on duplex |
2.5 Price and lifecycle cost
Indicative FOB China, USD per tonne, plate 4-12 mm, 3-15 t lot.
| Item | 1.4404 | 1.4462 | Comment |
|---|---|---|---|
| Metal price (indicative) | 3,150-3,550 | 2,850-3,300 | Duplex is often 5-15% cheaper per tonne |
| Thickness needed, 10 bar shell | 10 mm | 6 mm | Yield-driven design |
| Metal cost per m2 of shell | about 25.0-28.2 USD | about 13.6-15.7 USD | Duplex is roughly 45% cheaper in place |
| Welding cost | Baseline | +15-25% | WPS, consumables, control |
| Machining cost | Baseline | +25-40% | Tool wear and lower speeds |
| Life in chloride service | 3-8 years | 15-25 years | The lifecycle case |
The counter-intuitive result: duplex often wins on first cost as well as life, but only when the design is strength-limited and the fabricator is competent. Where the wall is set by corrosion allowance or handling rather than pressure, the thickness saving disappears and 1.4404 stays cheaper.
3. Applicable Duty and Selection Guide
3.1 Where 1.4404 remains correct
Tanks and vessels without pressure limitation, where corrosion allowance sets thickness
Service above 300 C, including hot oil, steam and flue-gas sections
Deep-drawn or heavily formed components needing 40% elongation
Dilute acid duty where neither grade performs and cost decides
Small-bore pipework and fittings in low-chloride cooling water
Applications requiring on-site weld repair without a WPS
3.2 Where 1.4462 is the better answer
Seawater cooling and service-water systems with flow above 1 m/s
Desalination high-pressure stages and brine reject lines
FGD absorber internals and slurry pipework
Pressure vessels and storage tanks where thickness is yield-limited
Heat exchanger tubes in chlorinated cooling water
Pulp mill digesters, bleach plant washers
Structural components needing high strength with corrosion resistance
Cargo tanks and chemical tanker pipework below 300 C
3.3 Three-step selection test
| Step | Check | Outcome |
|---|---|---|
| 1. Temperature | Service or excursion above 300 C? | If yes, stop: use 1.4404 or a heat-resisting grade |
| 2. Chloride + stress | Chloride present with tensile stress above 60 C? | If yes, 1.4462 is preferred for SCC resistance |
| 3. Thickness driver | Is wall thickness set by pressure (yield) rather than corrosion allowance? | If pressure-set, 1.4462 saves 30-45% metal |
If step 1 fails, no amount of PREN helps. If step 2 passes but step 3 fails, 1.4404 is cheaper and adequate - and that is roughly half of the enquiries we receive, which is why we quote both rather than defaulting to duplex.
4. What We Supply for Both Grades
20+ years of manufacturing, exports to 50+ countries, 200+ energy and petrochemical project deliveries.
| Product | 1.4404 range | 1.4462 range | Standard |
|---|---|---|---|
| Cold-rolled sheet | 0.3-3.0 mm | 0.4-3.0 mm | A240 / EN 10088-2 |
| Hot-rolled plate | 3.0-80 mm | 3.0-60 mm | A240 / EN 10028-7 |
| Coil and strip | 0.3-6.0 mm | 0.4-6.0 mm | A240 / A480 |
| Seamless tube | 6-219 mm OD | 6-219 mm OD | A213 / A269 |
| Welded tube | 12-630 mm OD | 12-630 mm OD | A249 / A312 |
| Bar and forgings | 10-300 mm | 10-300 mm | A276 / A182 |
Duplex orders ship with phase balance and ferrite content reported (typically 35-55% ferrite), impact test results at the specified temperature, PREN calculated from the actual heat analysis, and a welding procedure guide on request.
Send the design pressure, temperature, chloride level and drawing - we will calculate whether duplex thickness saving beats the 316L price gap and quote both with phase-balance documentation. Tell us whether your fabricator has a duplex WPS, because that decides the answer as much as the metallurgy.
FAQ: 1.4404 vs 1.4462
Is duplex always more expensive than 316L?
Per tonne, usually not - 1.4462 typically trades 5-15% below 1.4404 in China because it contains far less nickel. Per finished component, duplex is often 30-45% cheaper still, because its 450 MPa yield lets you use a thinner wall. The expensive version of duplex is the one fabricated without a controlled WPS.
What is the maximum temperature for 2205?
About 300 C for long-term service in most design codes, and many operators apply a lower limit of 250 C for sour or cyclic duty. Above that, sigma phase forms and toughness falls; a short-term excursion to 400 C is tolerable, continuous service is not. This limit applies regardless of the medium.
Can duplex replace 316L in a heat exchanger?
Yes, and it is the standard upgrade for chlorinated cooling water: higher PREN stops pitting at the tube wall, and higher strength allows thinner tubes with better heat transfer. What you must check is tube-to-tubesheet welding, where duplex needs ER2209 filler and controlled heat input.
Why does duplex need impact testing when 316L does not?
Because duplex contains ferrite and can form brittle phases; austenitic 316L has no such transition. Codes therefore require Charpy testing on duplex, typically 27 J minimum at the design minimum temperature, and the result tells you whether the heat treatment and welding were done correctly.
Does duplex resist chloride stress corrosion cracking?
Largely yes below about 150 C, which is its strongest advantage over 316L. 316L cracks in hot chloride under tensile stress; duplex does not, because the ferrite phase interrupts crack propagation. That is why duplex dominates hot chloride service even where pitting resistance alone would not justify it.
Can I weld 2205 to 316L?
Yes, with ER2209 or a nickel-based filler, and a procedure that limits heat input. Dissimilar joints should be qualified, and the duplex side needs the same interpass control as a duplex-to-duplex weld. Avoid welding duplex to carbon steel without a nickel barrier layer.
Which is better in stagnant seawater?
Neither is good. 316L fails quickly; duplex survives longer but suffers crevice corrosion and biofouling attack. Stagnant seawater requires 6Mo super austenitic or super duplex, plus design changes to keep water moving. Do not treat this as a 316L-versus-duplex question.
How do I verify duplex on delivery?
Three checks: PMI for chromium, molybdenum and nitrogen; ferrite content by metallography or ferritoscope within 35-55%; and phase balance with no sigma on a micrograph. A certificate alone is not enough - nitrogen below 0.14% and ferrite outside range are the two most common non-conformities.



Send Inquiry